Differences in Polishing Processes for Different Ferrule Diameters
Large Diameter Ferrule Face Grinding Process(FC/SC/ST-PC)
Process | Rubber Pad | Polishing Film | Auxiliary Liquids | Time | Pressure |
Degumming | PR5X-500-80 | GA5D 30um | Distilled water | 30s | Pressurization after 10 rpm |
Rough grinding | PR5X-500-80 | DR5D 5um | Distilled water | 30s | Pressurization at start |
Medium Grinding | PR5X-500-80 | DJ5D 1.5um | Distilled water | 30s | Pressurization at start |
Polishing | PR5X-500-80 | XF5D | Distilled water | 60s | Pressurized at start |
Cleaning | PR5X-500-80 | CF5D Cleaning buff | Distilled water | 12s | No pressurization |
Small Diameter Ferrule Face Grinding Process(LC-PC)
Process | Rubber Pad | Polishing Film | Auxiliary Liquids | Time | Pressure |
Degumming | PR5X-500-80 | GA5D 30um | —— | 30s | Pressurization after 10 rpm |
Convex Spherical Molding | PR5X-500-80 | DR5D 3um | Distilled water | 60s | Pressurization at start |
Polishing | PR5X-500-80 | XF5D | Distilled water | 60s | Pressurized at start |
Cleaning | PR5X-500-80 | CF5D Cleaning Buff | Distilled water | 12s | No pressurization |